Titanium Ti6Al4V Grade 23

钛合金
别名:TC4 / Ti-6Al-4V / Ti64

打印参数与力学性能(官方数据,可溯源)

设备/来源工艺状态层厚μm功率W扫描速度mm/s UTS MPaYS MPa延伸率%硬度密度g/cm³
Renishaw RenAM 500 LPBF Annealed-水平 (Horizontal XY) 60 — — 1 031 MPa ±5 MPa 938 MPa ±11 MPa 16% ±1% 348 HV0.5 ±7 HV0.5 —
Renishaw RenAM 500 LPBF Annealed-垂直 (Vertical Z) 60 — — 1 057 MPa ±4 MPa 986 MPa ±16 MPa 21% ±1% 344 HV0.5 ±6 HV0.5 —
Renishaw RenAM 500 LPBF Annealed-水平 (Horizontal XY) 90 — — 1 043 MPa ±3 MPa 961 MPa ±8 MPa 16% ±1% 351 HV0.5 ±5 HV0.5 —
Renishaw RenAM 500 LPBF Annealed-垂直 (Vertical Z) 90 — — 1 038 MPa ±8 MPa 969 MPa ±15 MPa 19% ±1% 351 HV0.5 ±7 HV0.5 —
Renishaw RenAM 500 LPBF Annealed-水平 (Horizontal XY) 60 — — 1 031 MPa ±5 MPa 938 MPa ±11 MPa 16% ±1% 348 HV0.5 ±7 HV0.5 —
Renishaw RenAM 500 LPBF Annealed-垂直 (Vertical Z) 60 — — 1 057 MPa ±4 MPa 986 MPa ±16 MPa 21% ±1% 344 HV0.5 ±6 HV0.5 —
Renishaw RenAM 500 LPBF Annealed-水平 (Horizontal XY) 90 — — 1 043 MPa ±3 MPa 961 MPa ±8 MPa 16% ±1% 351 HV0.5 ±5 HV0.5 —
Renishaw RenAM 500 LPBF Annealed-垂直 (Vertical Z) 90 — — 1 038 MPa ±8 MPa 969 MPa ±15 MPa 19% ±1% 351 HV0.5 ±7 HV0.5 —

工艺适配 · 钛合金

适用工艺:["gas_atomize", "prep", "plasma_atomize"]
不适用工艺:["water_atomize"]
反应性:high
加工难度:high
典型规格:22 条平台需求记录
加工难度:high
典型规格:5 条平台需求记录