Inconel 718

镍基
别名:IN718

打印参数与力学性能(官方数据,可溯源)

设备/来源工艺状态层厚μm功率W扫描速度mm/s UTS MPaYS MPa延伸率%硬度密度g/cm³
Renishaw RenAM 500 LPBF Solution treated and aged - Vertical (Z) 30 — — 1 414 MPa ±7 MPa 1 163 MPa ±11 MPa 27% ±3% 484 HV0.5 ±5 HV0.5 —
Renishaw RenAM 500 LPBF Solution treated and aged - Horizontal (XY) 30 — — — — — 466 HV0.5 ±8 HV0.5 —
Renishaw RenAM 500 LPBF As built - Horizontal (XY) 60 — — 1 048 MPa ±3 MPa 731 MPa ±3 MPa 34% ±2% 268 HV0.5 ±9 HV0.5 —
Renishaw RenAM 500 LPBF As built - Vertical (Z) 60 — — 951 MPa ±6 MPa 588 MPa ±5 MPa 40% ±3% 280 HV0.5 ±12 HV0.5 —
Renishaw RenAM 500 LPBF Solution treated and aged - Horizontal (XY) 60 — — 1 484 MPa ±5 MPa 1 280 MPa ±15 MPa 16% ±1% 474 HV0.5 ±11 HV0.5 —
Renishaw RenAM 500 LPBF Solution treated and aged - Vertical (Z) 60 — — 1 399 MPa ±6 MPa 1 196 MPa ±8 MPa 25% ±1% 480 HV0.5 ±12 HV0.5 —
Renishaw RenAM 500 LPBF Solution treated and aged - Vertical (Z) 90 — — 1 461 MPa ±8 MPa 1 221 MPa ±26 MPa 19% ±3% 479 HV0.5 ±9 HV0.5 —
Renishaw RenAM 500 LPBF Solution treated and aged - Horizontal (XY) 90 — — — — — 478 HV0.5 ±8 HV0.5 —
Renishaw RenAM 500 LPBF Solution treated and aged - Vertical (Z) 120 — — 1 461 MPa ±9 MPa 1 264 MPa ±19 MPa 22% ±4% 482 HV0.5 ±8 HV0.5 —
Renishaw RenAM 500 LPBF Solution treated and aged - Horizontal (XY) 120 — — — — — 484 HV0.5 ±10 HV0.5 —

工艺适配 · 镍基

适用工艺:["gas_atomize", "prep", "plasma_atomize"]
不适用工艺:["water_atomize"]
反应性:medium
加工难度:high
典型规格:16 条平台需求记录